With friendly support from
Hansueli Nydegger; www.nydegger-keramik.ch
wenzinger keramik; www.wenzinger-keramik.de
Martin Goerg
Marlen Schulze; www.fs-keramik.de/exponate-2006---marlen-schulze.html
Body 480 is a light to cream-coloured firing stoneware quality with 40 % chamotte 0 – 2.0 mm. The recommended firing range is 1000 °C – 1260 °C.
The plastic body is very suitable for building-up large-sized pieces. A rustic surface design is possible because of the coarse chamotte.
With friendly support from
Hansueli Nydegger; www.nydegger-keramik.ch
wenzinger keramik; www.wenzinger-keramik.de
Martin Goerg
Marlen Schulze; www.fs-keramik.de/exponate-2006---marlen-schulze.html
Firing colour | white-light cream | ||
Firing range (°C) | 1000 - 1260 | ||
Chamotte portion (%) | 40 | ||
Chamotte grain size (mm) | 0 - 2 | ||
DS (%)* | 4 | ||
Firing shrinkage | 1070 °C - 2% | 1140 °C - 3% | 1240 °C - 4% |
Water absorption | 1070 °C - 10% | 1140 °C - 7% | 1240 °C - 4% |
CTE x 10 -7 °C -1 | 20 °C - 500 °C (1240 °C) | 63 | |
Applications | Modelling | ||
Note | * DS = Dry shrinkage at 110°C |